Crystal system: triclinic
a: | 8.2989 (±0.0004) Å |
b: | 8.2986 (±0.0004) Å |
c: | 19.8768 (±0.0009) Å |
α: | 92.827 (±0.001)° |
β: | 99.124 (±0.001)° |
γ: | 90.142 (±0.001)° |
Starting materials: PbBr2 (99.999% trace metal basis), HBr (48 wt % in H2O, assay >99.99%), CH3OH (>99.9%), 2-(2-naphthyl)ethanamine (NEA, 95%)
Product: Colorless and laminar crystals.
Description: Dissolve PbBr2 (21.5 mg) in 0.5 mL of HBr (48%). Place CH3OH (1 ml) on top of the PbBr2 solution. Add 0.020 mL of NEA liquid into the CH3OH layer. Crystals would form in the solution overnight.
Method: Single-crystal X-ray diffraction
Description: Single-crystal X-ray diffraction data were collected using a Bruker D8 ADVANCE Series II at room temperature. The crystal structures were solved and refined by Shelxl and Olex software.
Starting materials: (NEA)2PbBr4 crystals, DMF, glass substrates
Product: Thin film on glass
Description: Dissolve the 2D single crystal into DMF at a concentration 6%∼10% relative to the total weight. Spin-coat at 3000 rpm for 30 s on glass substrates. Anneal in air at 100 °C for 10 min before measurement.
Method: Photoluminescence
Description: The photoluminescence spectra were measured using a Horiba-Jobi-Yvon LabRAM ARAMIS system, with a 325 nm He−Cd laser excitation. The laser beam was collimated and focused through a 40X UV objective onto the sample surface at room temperature.
Crystal system: triclinic
Photoluminescence peak position, nm |
---|
Starting materials: (NEA)2PbBr4 crystals, DMF, glass substrates
Product: Thin film on glass
Description: Dissolve the 2D single crystals into DMF at a concentration 6%∼10% relative to the total weight. Spin-coat at 3000 rpm for 30 s on glass substrates. Anneal in air at 100 °C for 10 min before measurement.
Method: Photoluminescence
Description: The photoluminescence spectra were measured using a Horiba-Jobi-Yvon LabRAM ARAMIS system, with a 325 nm He-Cd laser excitation. The laser beam was collimated and focused through a 40X UV objective onto the sample surface at room temperature. Refer to figure 5.
Starting materials: (NEA)2PbBr4 crystals, DMF, glass substrates
Product: Thin film on glass
Description: Dissolve the 2D single crystals into DMF at a concentration 6%∼10% relative to the total weight. Spin-coat at 3000 rpm for 30 s on glass substrates. Anneal in air at 100 °C for 10 min before measurement.
Method: UV-Vis absorption
Description: Optical absorption spectra were obtained using a Shimadzu UV-3600 spectrophotometer.