Crystal system: orthorhombic
Band gap (optical, transmission), eV |
---|
Starting materials: BABr (synthesized), PbBr2, HBr
Product: Colorless single crystals
Description: (BA)2PbBr4 crystals were synthesized by mixing BABr, and PbBr2 into a saturated HBr solution at a molar ratio of 2:1. Complete dissolution was achieved by heating to boiling with constant stirring for ~30 minutes. Upon slowly cooling, at a rate of 1°C/min to room temperature, the crystals precipitated. The crystals were removed by suction filtration and were dried in a vacuum.
Method: UV-vis absorption
Description: A Shimadzu UV-3101 UV-vis spectrophotometer was used to measure the absorption spectra.